Industry Type
Cement
Product Group
Lotherme
LOT 352
4
30
LOT 468
4
30
SHOVEL BOOM
HIGH TENSILE STEEL
LIMESTONE
TATA HITACHI 400
IMPACT AND ABRASION
CRACK DUE TO IMPACT AND ABRASION
1)GRINDING AND CLEANING THE SURFACE AREA.
2)GOUGING THE CRACK AREA
3)GRINDING THE SURFACE AREA.
4) CHECKING THE D P TEST.
5)THEN ROOT LAYER DEPOSITION WITH OUR LOTHERME 352(3.15 MM).
6)MULTI LAYER DEPOSITION WITH OUR
LOTHERME 352(4MM).
7)FINAL LAYER DEPOSITION WITH LOTHERME 468(4MM).
8) PLACING OF SUPPORTING BARS.